Answer Posted / karthikeyan..n
Injection pressure/injection rate too high
Barrel temperature too high
Insufficient clamping pressure
Mould sliding cores clearance too large Imprecise mould
alignment
Foreign material caused clearance on mould mating surface
Mould temperature too high Air venting design too large
Material over packed the mould cavity
Mould parting defects after age
Hopper temperature too high
| Is This Answer Correct ? | 1 Yes | 1 No |
Post New Answer View All Answers
HOW CAN WE MEASURE THE L SHAPE SURFACE OF THE MOMENT OF INERTIA AND SECTION MODULUS
Action plan to closr NCR (NON COONFORMANCE REPORTS)
what is rolling margin?( from view of machining process ) explain briefly
Will a steel cable become longer if it is heated while under load? Explain
What is the cause of cylindrical liner overheating?
i need rrb chennai JE mechanical last 2 year question papers Plz send me on this email id aaasaravanan@gmail.com
How do you convert 95 feet into square feet?
What is the difference between shear center flexural center of twist and elastic center?
What is fuel ratio ?
Is knowledge of properties of engineering materials is significant in pattern making why?
which power station plants r more efficient? which is less? which is most expensive and which is cheapest?
what is meant by absorptivity?
What is a radial-flow turbine?
Q. what @the interview exact Q&A is it correct
sir i m final year diploma(mech. engg)student, can i apply for psu,s as like sail, bhel,gail,dmrc.etc..if yes then give me detall about iton my e-mail id meatul90@rediffmail.com...thank you.........